ASTM B443 / ASME SB443 Alloy 625 Plate, Sheet and Strip (UNS N06625)
ASTM B443/B443M is an ASTM standard specification covering nickel-chromium-molybdenum-columbium alloy plate, sheet, and strip, widely known as Alloy 625 (Inconel 625, UNS N06625). This alloy contains 20–23% Cr, 8–10% Mo, and 3.15–4.15% Nb. Grade 1 material reaches yield strength up to 414 MPa (60 ksi). It delivers excellent corrosion resistance in seawater and various acid environments, with oxidation resistance up to 980°C (1800°F). ASME SB443 is the equivalent specification for ASME code-stamped pressure equipment.
1. Standard Scope & Designation
ASTM B443/B443M covers nickel-chromium-molybdenum-columbium alloy (UNS N06625, Alloy 625) plate, sheet, and strip in two grades:
- Grade 1: Annealed condition for high strength
- Grade 2: Solution-annealed condition for maximum corrosion resistance
Alloy 625 is a precipitation-hardenable Ni-Cr-Mo-Cb alloy combining high tensile strength, superior corrosion resistance and good fabricability.
| Form | Manufacturing Process | Standard Size Range |
| Plate / Sheet / Strip | Hot-rolled or cold-rolled from ingot or billet per standard | 0.010 in (0.25 mm) to 4 in (100 mm) |
Common stocked Alloy 625 plate size range: Thickness: 0.187–3.000 in (4.75–76 mm) Width: 48–96 in (1220–2440 mm) Sheet: 0.018–0.187 in (0.46–4.75 mm) Tolerances follow standard or purchaser agreement.
Scope Statement: This specification covers nickel-chromium-molybdenum-columbium alloy (UNS N06625) plate, sheet, and strip for use in general corrosive service and high-temperature applications requiring a combination of high strength, corrosion resistance, and oxidation resistance.
| Designation | Issuing Body | Unit System | Dimensional Reference | Latest Edition |
| ASTM B443 | ASTM International | Inch-Pound | ASTM A480/A480M | B443/B443M-19 (2024) |
| ASTM B443M | ASTM International | SI Metric | ASTM A480/A480M | B443/B443M-19 (2024) |
| ASME SB443 | ASME BPVC Section II Part B | Dual | ASTM A480/A480M | 2023 Edition |
2. Grades and Core Requirements
| Grade / UNS | Key Chemistry | Minimum Mechanical Properties |
| Grade 1 (N06625) | Ni min 58.0, Cr 20.0–23.0, Mo 8.0–10.0, Cb+Ta 3.15–4.15, Fe max 5.0, C max 0.10 | Annealed: TS ≥ 827 MPa (120 ksi), YS ≥ 414 MPa (60 ksi), El ≥ 30% |
| Grade 2 (N06625) | Same chemical composition as Grade 1 | Solution annealed: TS ≥ 690 MPa (100 ksi), YS ≥ 276 MPa (40 ksi), El ≥ 30% |
3. Chemical Composition (Weight %, Heat Analysis, ASTM B443 Table 1)
| Element | Specification | Notes |
| Ni | 58.0 min | Base alloy element, typical ~61% |
| Cr | 20.0–23.0 | Oxidation & corrosion resistance |
| Mo | 8.0–10.0 | Pitting / crevice corrosion resistance, solid-solution strengthening |
| Cb+Ta (Nb+Ta) | 3.15–4.15 | Precipitation strengthening (gamma-double-prime), IGC resistance |
| Fe | 5.0 max | Typical ~3.0% |
| C | 0.10 max | Typical ~0.03% |
| Mn | 0.50 max | — |
| Si | 0.50 max | — |
| Ti | 0.40 max | Controlled to preserve Nb precipitation |
| Al | 0.40 max | Controlled to preserve Nb precipitation |
| Co | 1.0 max | — |
| P | 0.015 max | — |
| S | 0.015 max | — |
4. Mechanical Property Requirements
All values represent minimum requirements. Tensile testing complies with ASTM E8/E8M.
| Grade & Condition | Heat Treatment | Min TS MPa (ksi) | Min YS MPa (ksi) | Min Elongation (%) |
| Grade 1 Plate, Annealed | ≥871°C (1600°F) | 827 (120) | 414 (60) | 30 |
| Grade 2 Plate, Solution Annealed | ≥1093°C (2000°F) | 690 (100) | 276 (40) | 30 |
| Grade 1 Sheet, Annealed | ≥871°C (1600°F) | 827 (120) | 414 (60) | 30 |
| Grade 2 Sheet, Solution Annealed | ≥1093°C (2000°F) | 690 (100) | 276 (40) | 30 |
5. Heat Treatment Guidelines
| Grade / Treatment | Temperature Range | Cooling Method | Purpose |
| Grade 1 Annealed | ≥871°C (1600°F) | Air cool or faster | Retain partial precipitation strengthening; high strength, moderate ductility |
| Grade 2 Solution Annealed | ≥1093°C (2000°F) | Water quench or rapid cool | Fully dissolve precipitates; maximum ductility and corrosion resistance |
| Stress Relief | 540–650°C (1000–1200°F) | Slow cool | Remove residual stress after welding or cold working |
6. Testing & Inspection Requirements
| Test Item | Requirement | Reference Standard |
| Heat Chemical Analysis | One test per heat, all elements meet table limits | ASTM B443 Table 1 |
| Tensile Test | One test per lot | ASTM E8 / E8M |
| Hardness Test | Rockwell B or Brinell by agreement | ASTM E18 / E10 |
| Intergranular Corrosion Test (Optional) | ASTM G28 Method A for sensitization check | ASTM G28 |
| Ultrasonic Examination | ASTM A578 or per purchaser agreement | ASTM A578/A578M |
| Visual & Dimensional Check | Thickness tolerance per ASTM A480; flatness by agreement | ASTM B443 / A480 |
7. Typical Applications by Industry
| Industry | Recommended Grade | Typical Service Application |
| Aerospace | Alloy 625 | Engine exhaust, thrust reversers, turbine shroud rings |
| Chemical Processing | Alloy 625 | Reactors, heat exchangers, piping for mixed acids and chlorides |
| Marine / Offshore | Alloy 625 | Seawater piping, subsea wellhead components, umbilical tubing |
| Oil & Gas | Alloy 625 | Sour gas wellhead parts, downhole tools, CRA cladding |
| Power Generation | Alloy 625 | Supercritical boiler components, FGD scrubber parts |
| Nuclear | Alloy 625 | Reactor internals, control rod drive mechanisms |
8. ASTM B443 Alloy 625 vs ASTM B575 Alloy C-276 (UNS N10276)
| Specification | ASTM B443 Alloy 625 | ASTM B575 Alloy C-276 |
| UNS Number | N06625 | N10276 |
| Ni Content | 58% min (typical ~61%) | Balance (typical ~57%) |
| Cr Content | 20.0–23.0% | 14.5–16.5% |
| Mo Content | 8.0–10.0% | 15.0–17.0% |
| Key Alloy Feature | Nb+Ta 3.15–4.15, precipitation hardenable | W 3.0–4.5, solid solution alloy |
| Grade 1 Minimum YS | 414 MPa | 283 MPa |
| PREN Range | ~45–55 | ~64 |
| High-Temp Performance | Excellent up to 980°C | Corrosion service limited to ~425°C |
| Best Fit | High strength + corrosion + oxidation resistance | Severe reducing acid & hot chloride environments |
Key Distinction: Alloy 625 (B443) delivers higher yield strength and superior high-temperature oxidation resistance. Alloy C-276 (B575) has a higher PREN value for extreme pitting resistance in concentrated chloride and reducing acid service.
9. Related Standards
| Standard | Description | Relation |
| ASTM B444 | Alloy 625 Seamless Pipe and tube | Matching tubular product standard |
| ASTM B705 | Alloy 625 welded pipe | Welded pipe version of Alloy 625 |
| ASTM B446 | Alloy 625 rod and bar | Bar stock for machining |
| ASME SB443 | ASME BPVC Section II Part B | Equivalent standard for ASME code stamped pressure vessels |
| ASTM G28 | Intergranular corrosion test for nickel alloys | Method A for sensitization testing |
| NACE MR0175 / ISO 15156 | SSC resistant materials for oil and gas | Approved for sour service |
| API 6A | Wellhead and Christmas tree equipment | Used for sour service trim and cladding |
10. Ordering Information
When placing an order for ASTM B443 plate/sheet/strip, provide the following information:
- Specification: ASTM B443 / ASME SB443
- Grade: Grade 1 (annealed) or Grade 2 (solution annealed)
- Product form: Plate, Sheet or Strip
- Dimensions: Thickness × Width × Length
- Heat treatment condition
- Surface finish: No.1, No.2D, No.2B or custom finish
- Optional test: ASTM G28 corrosion test (if required)
- Material certification: EN 10204 3.1 / 3.2 CMTR
- Quantity: Weight or area